CuNi 90/10 vs 70/30 (C70600 vs C71500): Which Copper-Nickel to Specify

Copper-nickel 90/10 (UNS C70600) vs 70/30 (UNS C71500): composition, strength, seawater velocity limits, standards and applications for pipes, tubes and bars.

By JPS Metal & Alloys · 19 Nov 2026 · 6 min read

Copper-nickel (CuNi, also called cupronickel) is the standard material for seawater piping, condensers, heat exchangers and firemains. The two grades most often specified are CuNi 90/10 (UNS C70600) and CuNi 70/30 (UNS C71500). Both resist seawater corrosion and biofouling. The main differences are strength, the flow velocity each can handle, and cost.

CuNi 90/10 vs 70/30 at a glance

PropertyCuNi 90/10 (C70600)CuNi 70/30 (C71500)
Nickel (%)9.0 to 11.029.0 to 33.0
Iron (%)1.0 to 1.80.4 to 1.0
Manganese (%)1.0 max1.0 max
CopperBalanceBalance
Typical tensile strength (annealed)about 275 MPaabout 360 MPa
EN designationCuNi10Fe1Mn, CW352HCuNi30Mn1Fe, CW354H
Relative costLowerHigher (three times the nickel)

Strength

The extra nickel makes 70/30 noticeably stronger than 90/10. That is why navies have traditionally used 90/10 for surface ships and 70/30 for submarines, where higher pressures need the stronger alloy. For most surface and onshore seawater systems, 90/10 has enough strength and is the economical choice.

Seawater velocity limits

Both alloys form a thin protective film in seawater, with general corrosion rates of about 0.0025 to 0.025 mm per year. That film is only stable below a design flow velocity. Above it, erosion corrosion starts, especially downstream of bends, tees and flanges. 70/30 tolerates higher velocities than 90/10. Typical design guidelines are:

Service90/10 (m/s)70/30 (m/s)
Condensers and heat exchangers, once-through2.43.0
Condensers and heat exchangers, two-pass2.02.6
Piping up to 76 mm ID, long-radius bends2.52.8
Piping 77 to 99 mm ID, long-radius bends3.23.5

Source: Copper Development Association design guidelines. Larger pipe diameters allow higher velocities. Your piping designer should confirm the limit for each line size.

Where each grade is used

  • CuNi 90/10 (C70600): seawater cooling and firewater piping, ship and offshore piping systems, desalination plant piping, condenser and heat exchanger tubes, hull sheathing and splash-zone cladding.
  • CuNi 70/30 (C71500): high-velocity condenser tubes, heat exchangers in power plants and MSF desalination, high-pressure seawater lines, pump and valve parts, and hollow bars machined into components that need extra strength.

Standards to specify

Common specifications are ASTM B111 for condenser and heat exchanger tubes, ASTM B466 for seamless pipe, ASTM B467 for welded pipe, ASTM B151 for rod and bar, and ASTM B171 for plate. For offshore 90/10 piping systems, EEMUA 144 (pipes), 145 (fittings) and 146 (flanges) are widely used. In Europe, specify the EN material number (CW352H or CW354H) with the relevant EN product standard.

How to choose

Choose 90/10 for most seawater piping and heat exchangers where velocities stay within the limits above. It costs less and has excellent resistance to biofouling. Choose 70/30 where you need higher strength, higher flow velocity or better erosion resistance, for example in high-velocity condensers or pressure-retaining parts. Both alloys are sensitive to sulphide-polluted water, so pay extra attention to commissioning and to lay-up in polluted harbours.

CuNi 90/10 and 70/30 from JPS Metal & Alloys

We supply CuNi 90/10 and 70/30 round bars, hollow bars, plates, seamless pipes and tubes, fittings and flanges from Mumbai, with EN 10204 3.1 mill test certificates and optional third-party inspection. We export to the GCC, Europe, Singapore and the USA. Send your grade, size and quantity for a quote.

Frequently Asked Questions

Is CuNi 70/30 better than 90/10?
Not in every case. 70/30 is stronger and tolerates higher seawater velocities, but it costs more. 90/10 is the usual choice for seawater piping and heat exchangers within normal velocity limits.
What is C71500 material?
C71500 is the UNS number for 70/30 copper-nickel: about 30% nickel with small amounts of iron and manganese, balance copper. Its EN equivalent is CuNi30Mn1Fe (CW354H).
What is the UNS number for CuNi 90/10?
CuNi 90/10 is UNS C70600, EN CuNi10Fe1Mn (CW352H).

Need material to a specification? Send your grade, size and quantity.

Request a Quote →